Home / Articles / Buying custom alloy ingots
Buying guide

How to Buy Custom Cast Alloy Ingots: Composition, Form and Papers

A custom ingot is a specification, not a catalogue line. This guide sets out the numbers to fix before the heat is melted: composition basis and element roles, grade data, ingot form and unit weight, the melting records, and the inspection plan behind the certificate.

1. Start with the part, not the grade

Write down the service before the grade: load, speed, working temperature, lubrication, the material it runs against, and the failure you are trying to stop. A zinc-aluminum bearing that failed by wear is a different enquiry from one that failed by fatigue spalling; the first points to hardness and a zinc alloy, the second may point back to babbitt or to a bronze with better embeddability.

Once the duty is written down, the grade follows. If it does not follow, that is the point to ask the foundry rather than to pick a name from a list.

2. What the RFQ must fix

Four lines decide whether two quotations are comparable.

Composition basisSay whether you are giving a standard grade, a composition window or only a performance target. The three lead to different melting and testing routines.
Ingot formShape, unit weight, bundle weight and pallet footprint. This has to match your charging bucket, crane and furnace, not a catalogue.
Packing and markingStrapping, bundle weight, grade and heat number on the bundle, and where the documents travel.
EvidenceCertificate per heat, sampling plan, mechanical tests, third-party inspection if your quality system requires it.

Quantity and delivery date belong in the same enquiry, but they are the easy part. The four lines above are what separates two quotations that look identical on price.

3. Composition: what is controlled, and why

A grade name is a shorthand for a set of element ranges. When you write your own window, it is worth knowing which element does which job, because that is where the argument starts when a heat comes back out of specification.

Element Role in ZA303 (Zn-Al) Role in ZL205A (Al-Cu-Mn)
ZnMatrix; balance of the alloyImpurity, held low
Al25-28%; raises strength and hardnessMatrix
CuRaises strength, hardness and dimensional stability4.6-5.3%; main strengthener, widens the freezing range
MgSmall addition; refines structure, improves dimensional stabilityNot an alloying element
Mn-0.3-0.5%; strengthens and controls iron
CdImpurity, held low0.15-0.25%; ageing response
Ti-0.15-0.35%; grain refinement
B, Zr-Small additions for grain control, per GB/T 1173

ZL205A ranges are the nominal GB/T 1173 ranges; ZA303 is a company grade, so its full window is stated on the certificate for the heat supplied.

That distinction matters. ZA303 is not a GB or ASTM designation; its composition is controlled by the supplier's specification, which is why the certificate, not the grade name, is the document that tells you what you bought. ZL205A is a standard designation, but its range is wide enough that a window on paper does not guarantee a casting of 500 MPa - gating, shrinkage control and the T5 or T6 condition carry as much of the result as the chemistry.

Four rules keep a window checkable: name every element with a minimum and a maximum; state the sampling point and the method; say what happens at the edge of the window before the heat is made; and do not copy a competitor's certificate as your own window.

4. Grade data you can quote

Published typical values, not design allowables.

Grade Family Tensile Rm Hardness Density Service limit / use
ZA303Zn-Al300-450 MPaHB 90-120about 2/3 of copperbelow 150 °C continuous; bearings, bushings, liner and slide plates, worm wheels
ZA-27Zn-Alhigher than ZA-12--below 150 °C; bearing and wear parts where strength matters
ZA-12Zn-Allower than ZA-27--below 150 °C; the most castable of the ZA family
ZL205AAl-Cu-Mn436 as cast / 510 T5 / 470 T6HB ~131 in T52.82 g/cm³load-bearing structural parts; T5/T6 required for the 500 MPa class
ZL205A tensile, yield and elongation as cast, in T5 and in T6
ZL205A by condition: typical values from public literature on separately cast bars - not a design allowable

Read the ZL205A row carefully: the same grade gives 436 MPa as cast and 510 MPa in T5, with elongation moving from 3.3% to 8.1%. That spread is the reason a specification that names only the grade is not a specification of the part.

5. Friction and wear: the zinc-aluminum case

The argument for ZA303 is not that it is harder than bronze across the board; it is the combination of friction, wear loss and density. Against steel its friction coefficient is about 0.08-0.12, against roughly 0.15-0.20 for copper alloys. Wear loss in comparable sliding pairs is about one quarter, and service life in bushings is typically two to three times that of tin bronze.

ZA303 friction coefficient, wear loss and service life compared with copper alloys
ZA303 against copper alloys: friction, wear loss and service life as relative values from published data

Where that pays: large slow-shaft bearings on mills and kilns, crusher and ball-mill bushings, and slide plates on heavy face-contact pairs. Where it does not: continuous service above about 150 °C, high-speed duty with an already thin oil film, and very heavy impact, where babbitt's embeddability is still the safer choice. Aging matters too - a high-aluminum zinc casting that is not aged keeps changing size and loses its fits.

6. Ingot form and unit weight

Ingot shape is a handling decision. Trapezoid ingots stack and recharge well; square ingots pack densely in a storage bay; round ingots suit some induction furnaces. Notches help an ingot break cleanly and sit stable on a stack.

Trapezoid, square and round ingot forms with W, H and D dimensions
Ingot forms: trapezoid, square and round; unit weight, length and notch depth are agreed per order
FormCharging StackingBest for
Trapezoideasy, self-locatingstablegeneral recharging
Squaregooddensestorage and transport
Roundrolls, hand-fedlimitedinduction furnaces

Unit weight should be matched to the charging bucket and melt rate. Too heavy and the ingot bridges in the throat of the furnace; too light and oxidation losses climb. Bundle weight and pallet footprint matter just as much on site: they decide whether your forklift or crane can move the delivery without breaking it down. The ingots must be dry and free of coolant residue before charging, and the bundle marking has to survive outdoor storage long enough for the receiving inspection to read it.

7. Melting and casting records

A custom ingot is only as good as the records behind it. For each heat, the foundry should be able to show:

  • charge weight and charge composition
  • alloying additions and the order they were made in
  • spectrographic analysis of a sample cast with the heat, before pouring
  • degassing and grain refinement
  • pouring temperature, recorded per heat
  • mould condition and coating
  • ingot weight check and bundle marking
  • the heat number carried through to the bundle and the certificate

Ask for those records before you need them. A foundry that can produce the heat log can answer a failure question in an afternoon; one that cannot will answer it with a new quotation.

8. Inspection plan and certificate

ItemMethod FrequencyRecord
Chemical compositionspectrographic analysis of a sample cast with the heatevery heatcertificate of analysis
Tensile, yield, elongationseparately cast test barper heat or as agreedtest report
HardnessHB at an agreed locationas agreedtest report
Internal soundnessX-ray or ultrasonic, critical partson requestinspection report
Weight and dimensionsweighing and gaugeeach bundlepacking list
Markingvisual: grade, heat number, bundle weighteach bundleshipping record

If your incoming inspection needs a retained sample, say so in the enquiry; it is much easier to set aside at the heat than to recover later.

9. Why a trial heat comes before the batch

A trial ingot confirms four things at once: the composition meets the window, the melt flows well enough for your casting, the shrinkage pattern is manageable, and the ageing or heat-treatment response is where you expect it. None of those is proved by a certificate alone.

The economics are simple. A scrapped heat costs the metal, the melting time and the delay; a trial batch costs a fraction of that and settles the arguments before they reach the shop floor. Trial quantity is agreed per ingot shape and furnace charge, not quoted from a price list.

10. Three mistakes buyers make

Treating ZL205A as a zinc alloy. It is an Al-Cu-Mn casting aluminium alloy, with a different density, casting behaviour and heat treatment from the ZA family. Ordering it as "zinc-aluminium" gets the wrong melt and the wrong process route.

Copying babbitt clearance onto a ZA303 drawing. ZA303 expands more than babbitt, so the clearance has to be recalculated for the working temperature; the old drawing usually comes out too tight.

Buying on the grade name only. For a defect-sensitive alloy, the grade meeting specification and the casting meeting specification are two different things. Ask how the gating was designed, where the test bar came from and which condition the part is in.

11. What drives the price

Custom ingot prices move with four things: the alloy content, especially copper and aluminium; the ingot mould and unit weight, because a short run in a special shape costs more per tonne than a standard one; the testing regime, from spectrographic analysis alone to mechanical tests and third-party inspection; and the batch size and packing.

That is why a useful enquiry gives the composition basis and the annual or per-order quantity together. A quotation against a grade name alone is a guess on both sides.

Questions we get

Can you melt to our own composition rather than a standard grade?

Yes. Send the element ranges and the sampling method, and every heat is checked against that window by spectrographic analysis before the ingots are released.

What is the smallest trial batch you will melt?

It depends on the ingot shape and the furnace charge. Trial quantities are possible; the exact weight is agreed in the quotation.

Can ingots and castings come from the same heat?

Yes. The same heat can produce ingots and be poured into rough castings, which avoids a second melt and its composition drift and losses.

Which grades can you supply as ingots?

Zinc-aluminum ZA303, ZA-27 and ZA-12, and aluminum alloys including ZL205A. Other compositions are melted to the customer's drawing or specification.

Do you cast a separate test bar?

Yes, separately cast test bars can be agreed in the order. The certificate states whether the bar was cast separately or cut from a part, because the two are not the same claim.

What is the weight tolerance on an ingot?

Each bundle is weighed and marked. Individual ingot weight and bundle weight follow the mould and the furnace charge, and both are agreed in the order.

How are the ingots packed?

Strapped bundles on pallets, with grade, heat number and bundle weight marked. Bundle weight and pallet size are agreed per order.

Do you issue a certificate of analysis with each shipment?

Yes, one certificate per heat, showing the measured composition and any mechanical tests agreed in the order. Third-party inspection can be arranged.

Related casting and ingot pages

Custom cast alloy ingots (ZA303 / ZL205A) · Zinc-based vs aluminum-based ingots · ZA303 grade data · Aluminum alloy castings

Need a quote or a custom part?

Send your drawing, sample photo or specification - we reply within 1 business day.

Request a Quote