Shenyang Yuheng Metal Manufacturing
Wear-resistant alloy castings & bearings
HomeProductsArticlesAboutAlloy GradesContact
EN

Home / Alloy Grades / Cast Copper Alloy

C93800

High-Leaded Tin Bronze (78-7-15)  |  ASTM B584 / B505  |  UNS C93800  |  SAE 67 (J461 / J462)

We cast and machine this grade. Bushings, bearings, valve bodies and custom parts to drawing  View products

Chemical Composition (%)

Cu75.0-79.0
Sn6.3-7.5
Pb13.0-16.0
Zn0.8 max
Fe0.15 max
Ni1.0 max
Sb0.80 max
S0.08 max
P0.05 max
Al / Si0.005 max each

Limits as published for the ASTM designation; single values are maximums unless shown as a range. Cu is stated as the balance.

Mechanical & Physical Properties

Tensile strength179 MPa min (26 ksi)
Yield strength97 MPa min (14 ksi)
Elongation12% min
Hardness58 HB (typical)
Density9.24 g/cm³
Machinability80 (free-cutting brass = 100)
Modulus of elasticity72 GPa
Impact strengthabout 7 J (5 ft-lb)

Minimum values are standard limits; hardness and machinability are typical values unless marked as minimum.

C93800 composition ranges
Published composition ranges for C93800 (bar = midpoint, whisker = range).

Typical Applications

general-service bearingsbushingsmine-water pump partsmoderate-pressure fittingswearing platesthrust washers

Grade Overview

C93800 is a high-leaded tin bronze: 75-79% copper, 6.3-7.5% tin and 13-16% lead. The lead is the point of the alloy. It sits as a soft, continuous phase through the matrix, giving excellent conformability, embeddability and machinability - a rating of 80, the highest in this family - at the cost of strength and toughness. Published limits are only 179 MPa minimum tensile strength, 97 MPa minimum yield and 12% minimum elongation, with a typical hardness of 58 HB and an impact strength of about 5 ft-lb.

That trade is deliberate and useful. A high-lead bronze is chosen for bearings that must run in dirty or poorly aligned service, where the bearing should embed grit and conform to the shaft rather than score it. It is also used for mine-water pump parts and moderate-pressure fittings where machinability and pressure tightness matter more than load capacity. It is not a structural alloy, and it should not be specified where the part must carry high load, shock or bending.

Cast copper alloy family strength and hardness
Strength and hardness across the cast copper alloy family, from published ASTM limits.

Microstructure and Behaviour

A copper-tin matrix with a substantial network of lead particles. The lead network is what gives the low friction, the embeddability and the free-machining behaviour; it also lowers strength and makes the alloy sensitive to overheating. Castings are used as-cast, with no hardening treatment.

Standards and Equivalents

C93800 is ordered to ASTM B584 for sand castings and B505 for continuous cast; SAE 67 (J461/J462) is the traditional designation. The nearest GB/T 1176 grade is ZCuPb15Sn8, an approximate match on lead and tin but not an exact composition. Because the alloy is lead-rich, confirm the regulatory position before specifying it for potable water, food equipment or consumer products.

Selecting C93800

Choose C93800 for bearings and bushings in dirty, misaligned or shock-prone service, for mine-water pump parts and for moderate-pressure fittings where machinability and conformability dominate. Against C93200 it has much more lead (13-16% versus 6-8%) and lower strength; it embeds better and machines faster but carries less load. Against C93700 it is softer and weaker but even more forgiving of dirt. Against C90700 it trades load capacity for conformability. Never use it as a structural bronze.

How to Specify C93800 on a Drawing

Casting and Machining Notes

High-lead bronze is fluid and casts detail well, with low shrinkage and high casting yield - it is one of the easier copper alloys to cast. The risks are lead segregation in heavy sections and overheating, which coarsens the lead network and lowers properties. Keep pouring temperature controlled and stir the melt before pouring. Machining is the alloy's strength: it cuts freely, breaks chips and takes a good finish.

Bearing duty and lubrication

C93800 is a conformable bearing alloy, not a high-strength one. Design for generous wall thickness, good oil distribution and a running-in period; the lead network will conform to slight shaft misalignment and embed grit that would score a harder bronze. Where the load is high or the shock severe, move to C90700 or an aluminum bronze and solve the dirt problem with sealing rather than with embeddability.

Frequently asked questions about C93800

What is C93800 used for?

General-service bearings and bushings, mine-water pump parts, moderate-pressure fittings, wearing plates and thrust washers. It is chosen for conformability, embeddability and machinability rather than strength.

C93800 or C93200?

C93800 contains 13-16% lead against roughly 6-8% in C93200, so it is softer, weaker (179 MPa versus about 240 MPa minimum) and even more forgiving of dirt, but it carries less load. Use C93800 for dirty, slow, misaligned duty; C93200 where more strength is needed.

Can C93800 be used in drinking water?

Normally no. With 13-16% lead, the alloy is outside drinking-water and food-contact limits in most markets. Confirm the regulation for the destination before specifying it, and expect to use a lead-free bronze instead.

Why is the machinability rating so high?

The lead network lubricates the tool and breaks the chip, so C93800 cuts at a rating of about 80 against free-cutting brass - faster and with better finish than any other bronze in this family.

Is C93800 strong enough for a structural part?

No. Minimum tensile strength is 179 MPa and impact strength is about 5 ft-lb. It is a bearing and fitting alloy, not a structural one; use a manganese bronze, aluminum bronze or steel where the part carries structural load.

How should C93800 castings be fed?

The alloy is fluid with low shrinkage and high yield, so feeding is easier than for high-tin bronze. Watch lead segregation in heavy sections and avoid overheating, which coarsens the lead network and reduces properties.

Data compiled from published ASTM B584, B505/B505M and B271 limits and from mill specification sheets (Diversified Bronze, Concast, St. Paul Foundry); for selection reference only. Ordering is subject to the standard and the mill certificate. Data source: Shenyang Yuheng Metal Manufacturing Co., Ltd. — yuhengmetal.com.

Related grades

C93200 · C93700 · C90700 · C90500  |  All 62 grades in the library

← Back to Alloy Grades