Chemical Composition (%)
| Cu | 78.0-82.0 |
|---|---|
| Sn | 9.0-11.0 |
| Pb | 8.0-11.0 |
| Zn | 0.80 max |
| Fe | 0.70 max (0.35 max steel-backed) |
| Ni | 1.50 max |
| P | 0.50 max |
| Sb | 0.50 max |
| Al | 0.005 max |
| Si | 0.005 max |
Limits as published for the ASTM designation; single values are maxima.
Mechanical & Physical Properties
| Tensile strength | >= 241 MPa (35 ksi) |
|---|---|
| Yield strength (0.5% ext.) | >= 138 MPa (20 ksi) |
| Elongation (2 in.) | >= 10% |
| Hardness | about 60 HB (typical) |
| Density | 8.86 g/cm3 |
| Melting range | 762-929 C |
| Electrical conductivity | 10% IACS |
| Machinability | free-machining, leaded bronze |
Mechanical values are standard minima; hardness is typical.
Typical Applications
Bushings and bearings for high speed and heavy pressure, marine and railway shaft bearings, rolling-mill bearings, pump and crusher bearings, and sliding surfaces where dirt or grit is expected. It also resists sulphite liquors, which keeps it in use in paper-mill equipment.
Grade Overview
C93700 - SAE 64, or 80-10-10 - is a high-leaded tin bronze: about 80% copper, 10% tin and 10% lead. The high lead content is deliberate. Lead does not dissolve in the copper matrix; it sits as a distributed soft phase that lets the bearing conform to a slightly misaligned shaft, embed grit and metal particles instead of scoring the journal, and keep working when the oil film is interrupted. That combination is why it has long been the standard choice for heavily loaded bearings that run at speed or with uncertain lubrication.
The same structure sets its limits. Lead lowers strength and ductility, the alloy is not weldable, and it is a bearing material rather than a structural one. Where a part must carry load and also resist bending or shock, an aluminum bronze or a high-strength brass is the better answer.
Standards and Equivalents
ASTM B505 covers continuous-cast bar and ASTM B271 centrifugal castings; SAE lists the alloy as SAE 64, and QQ-C-390 E10 is the older federal call-out. Chinese GB/T 1176 designates the nearest grade ZCuPb10Sn10, and EN 1982 lists CuPb10Sn10. For steel-backed bearings, ASTM limits iron to 0.35% max - tighter than the general casting limit - because the lining is bonded to a steel shell and excess iron weakens the bond.
| UNS | C93700 |
|---|---|
| Common name | 80-10-10 / SAE 64 |
| ASTM | B505 (continuous cast) / B271 (centrifugal) |
| Federal | QQ-C-390 E10 |
| China | ZCuPb10Sn10 (GB/T 1176) |
| Europe | CuPb10Sn10 (EN 1982) |
Equivalent grades are close in composition and duty, not identical. Order and certify to the standard named on the drawing.
How to Specify C93700 on a Drawing
- Write "C93700 (SAE 64)" and name the standard; "80-10-10" alone is used loosely for similar high-lead bronzes.
- For bimetal or steel-backed shells, state the bonding method and lining thickness, and require the steel-backed iron limit.
- Add a soundness requirement: lead-rich alloys are prone to porosity and lead segregation, and a bearing with internal voids fails early.
- Do not ask for weld repair or build-up; the alloy is not weldable in practice.
- For bearings, give the shaft diameter, clearance range, lubrication method and load direction, so the groove and oil holes are placed in the loaded zone.
Selecting C93700
Choose C93700 where the bearing must tolerate misalignment, dirt or lubrication lapses at high load and speed. For general-purpose bearing duty with better strength and machinability, C93200 is the usual pick. For even higher lead and greater conformability at lower strength, C93800 goes further in the same direction. Where strength and corrosion resistance dominate, aluminum bronze C95400 is the alternative, at the cost of embeddability.
Casting and Machining Notes
C93700 machines freely but generates lead-bearing chips and dust, so local extraction and the usual lead-hygiene controls apply in the machine shop, including waste segregation. In casting, the risks are lead segregation and shrinkage porosity: keep pouring temperature under control, avoid long holding times, and inspect heavy sections. Bearings should be designed with a proper oil groove, adequate clearance and a smooth journal finish; the alloy forgives a little misalignment, not a dry start.
Frequently asked questions about C93700
What does 80-10-10 mean?
It is the nominal composition: about 80% copper, 10% tin and 10% lead. The formal designation is UNS C93700, and SAE lists the same alloy as SAE 64.
Why use C93700 instead of C93200?
C93700 carries more lead, so it conforms to misalignment and embeds dirt better, and it keeps running longer when lubrication is marginal. C93200 is stronger, harder and easier to machine, and is the better general-purpose choice. Pick C93700 for high speed, heavy pressure or dirty service.
Is the lead in C93700 a health issue in the workshop?
Yes during machining and fettling. Lead-bearing chips and dust require local extraction, personal protection and controlled waste disposal, and some markets restrict leaded copper alloys in certain products. Casting and machining shops should apply the lead-hygiene rules that apply locally.
What is the difference between C93700 and C93800?
C93800 carries more lead (around 15%) and less tin, so it is softer, more conformable and weaker. It suits very heavily misaligned or poorly lubricated bearings and older equipment. C93700 is the more common general high-lead bearing bronze.
Data compiled from published ASTM B505/B505M, B584 and B148 limits and from mill specification sheets; for selection reference only. Ordering is subject to the standard and the mill certificate. Data source: Shenyang Yuheng Metal Manufacturing Co., Ltd. — yuhengmetal.com.
Related grades
C93200 · C83600 · ZCuPb10Sn10 (GB/T 1176) | All grades in the library