C93200

SAE 660 Bearing Bronze (Leaded Tin Bronze)  |  Cast Copper Alloy  |  ASTM B505 / B271  |  UNS C93200

We make this grade. Copper alloy castings and machined bushings to this specification, with certificate of analysis  View products

Chemical Composition (%)

Cu81.0-85.0
Sn6.3-7.5
Pb6.0-8.0
Zn2.0-4.0
Fe0.20 max
Ni1.00 max
Sb0.35 max
Al0.005 max
Si0.005 max

Limits as published for the ASTM designation; single values are maxima.

Mechanical & Physical Properties

Tensile strength>= 241 MPa (35 ksi)
Yield strength (0.5% ext.)>= 138 MPa (20 ksi)
Elongation (2 in.)>= 10%
Hardnessabout 65 HB (typical)
Density8.91 g/cm3
Melting range854-977 C
Electrical conductivity12% IACS
Machinabilityabout 70% of free-cutting brass

Mechanical values are standard minima; hardness is typical.

Typical Applications

general-purpose bushingsthrust washersroll-neck bearingspump bushingsmachine-tool bearingshydraulic press bushingstrunnion bearingsvalve guides

The usual duty is a rotating or oscillating shaft under steady load: general-purpose bushings, thrust washers, roll-neck bearings in rolling mills, pump and water-pump bushings, machine-tool spindle bearings, hydraulic press bushings and trunnion bearings. It is also the common repair choice, because it can be machined to fit a worn shaft without changing the housing.

Grade Overview

C93200 - sold in the United States as SAE 660 - is the general-purpose bearing bronze of the American market. Its composition is built around roughly 7% tin, 7% lead and 3% zinc in a copper base: tin gives the matrix strength and wear resistance, lead sits in the structure as a dispersed soft phase that provides lubricity and lets the alloy tolerate a brief loss of oil film, and zinc improves fluidity and economy. The result is an alloy that machines freely, runs quietly against a steel shaft and carries moderate loads at moderate speeds.

In practice C93200 is the grade most US purchasers name when they ask for "bearing bronze" without a drawing number. It is stocked as continuous-cast bar and tube to ASTM B505 and produced as centrifugal castings to ASTM B271 for larger rings and sleeves. Continuous casting gives a fine, uniform grain and a sound section, which is why bar stock is the usual starting point for bushings and thrust washers. It is not a high-strength alloy: minimum tensile strength is around 241 MPa and hardness around 65 HB, so it suits steadily loaded, well-lubricated bearings rather than shock or edge loading. It is not weldable and should not be specified where the part must also act as a structural member.

Standards and Equivalents

C93200 is controlled by ASTM B505/B505M for continuous-cast copper alloy rod and bar, and by ASTM B271 for centrifugal castings. SAE J461/J462 list it as SAE 660, and the older federal specification QQ-C-390 E7 still appears on drawings. Its closest Chinese designation is ZCuSn6Zn6Pb3 in GB/T 1176, and the nearest European grade is EN 1982 CuSn7Zn4Pb7 (CC493K). These are close in composition and duty, not identical: element ranges, impurity limits and mechanical minima differ, so a certificate to one standard cannot be read as compliance with another. When a US drawing calls ASTM B505, supply and certify to ASTM B505.

UNSC93200
SAE660 (J461 / J462)
ASTMB505 (continuous cast) / B271 (centrifugal)
FederalQQ-C-390 E7
ChinaZCuSn6Zn6Pb3 (GB/T 1176)
EuropeCuSn7Zn4Pb7 / CC493K (EN 1982)

Equivalent grades are close in composition and duty, not identical. Order and certify to the standard named on the drawing.

How to Specify C93200 on a Drawing

Selecting C93200

Choose C93200 for general-purpose bearings running at moderate load and speed with reliable lubrication. Where corrosion resistance and pressure tightness matter more than bearing duty - valve bodies, pump housings, flanges - C83600 red brass is the more usual choice. Where the bearing runs faster, carries edge load or works with intermittent lubrication, the higher-lead C93700 conforms and embeds debris better. Where load is heavy and speed low, C86300 carries far more. Where strength plus seawater corrosion resistance is needed, C95400 aluminum bronze is the right move.

Casting and Machining Notes

C93200 is one of the easiest cast copper alloys to machine, rated at about 70% of free-cutting brass, and it takes a good finish with sharp tooling and light finishing cuts. In the foundry the main concerns are lead segregation and gas porosity, so melt temperature and pouring practice need control; continuous casting avoids many of the feeding problems of sand castings. Bearing design matters as much as the alloy: provide a lubrication groove and holes that actually reach the loaded zone, allow clearance for thermal growth, and avoid sharp transitions that create edge loading. The alloy is not weldable, so worn parts are re-machined or replaced, not built up.

Frequently asked questions about C93200

Is C93200 the same as SAE 660?

Yes. SAE 660 is the SAE designation for the same copper alloy that ASTM and the Copper Development Association call C93200. Drawings may also say "bearing bronze", "SAE 660 bronze" or "932 bronze"; they all point to this composition.

How does C93200 differ from C83600?

C83600 (85-5-5-5 red brass) carries less tin and more zinc and is used mainly for pressure-tight castings such as valves, flanges and pump housings. C93200 carries more tin, which makes it harder and more wear-resistant, and it is used for bearings and bushings. C83600 casts and pressure-tests better; C93200 bears load better.

Can C93200 be welded?

No. Welding is not recommended: the lead phase volatilises and the structure cracks. Repairs are made by replacing the part or, in non-critical areas, by brazing, and even brazing is limited. Design for replaceable bushings rather than weld repair.

What is the difference between ASTM B505 and ASTM B271?

B505 covers continuous-cast rod and bar; B271 covers centrifugal castings. Both may be C93200, but casting process, available section size and test requirements differ, so order to the standard that matches the form you are buying.

Data compiled from published ASTM B505/B505M, B584 and B148 limits and from mill specification sheets; for selection reference only. Ordering is subject to the standard and the mill certificate. Data source: Shenyang Yuheng Metal Manufacturing Co., Ltd. — yuhengmetal.com.

Related grades

C83600 · C93700 · ZCuSn6Zn6Pb3 (GB/T 1176)  |  All grades in the library