Chemical Composition (%)
| Cu | 84.0-86.0 |
|---|---|
| Sn | 4.0-6.0 |
| Pb | 4.0-6.0 |
| Zn | 4.0-6.0 |
| Ni | 1.00 max |
| Fe | 0.30 max |
| Sb | 0.25 max |
| P | 0.05 max |
| S | 0.08 max |
| Al | 0.005 max |
| Si | 0.005 max |
Limits as published for the ASTM designation; single values are maxima.
Mechanical & Physical Properties
| Tensile strength | >= 207 MPa (30 ksi) |
|---|---|
| Yield strength (0.5% ext.) | >= 97 MPa (14 ksi) |
| Elongation (2 in.) | >= 20% |
| Hardness | about 62 HB (typical) |
| Density | 8.80 g/cm3 |
| Melting range | 853-1009 C |
| Electrical conductivity | 15% IACS |
| Machinability | about 84% of free-cutting brass |
Mechanical values are standard minima; hardness is typical.
Typical Applications
Low-pressure valves and valve bodies, flanges, pipe fittings, pump housings and impellers, water-supply components, marine and industrial hardware, and general engineering castings that must be pressure-tight. It is also used for decorative and architectural castings where a warm red colour is wanted.
Grade Overview
C83600, known across the US trade as 85-5-5-5, is the standard leaded red brass for castings. The name records the nominal composition: about 85% copper with 5% each of tin, lead and zinc. That balance explains its popularity: tin gives strength and corrosion resistance, lead improves machinability and pressure tightness, and zinc lowers cost while improving fluidity in the mould.
It is a casting alloy first and a bearing alloy second. Its value in valves, flanges, pump bodies and water fittings is that it fills thin sections, reproduces detail and holds pressure without leaking. Sand casting to ASTM B584 is the normal route; continuous-cast bar to ASTM B505 is available when bar stock is wanted. Mechanically it is modest - minimum tensile strength around 207 MPa, yield around 97 MPa, elongation about 20% and hardness near 62 HB - but it is tough enough for pressure-containing bodies and machines freely.
Standards and Equivalents
C83600 is specified in ASTM B584 for sand castings for general applications and in ASTM B505 for continuous-cast bar; the ingot is covered by ASTM B62, and SAE J461/J462 and QQ-C-390 also list the alloy. Chinese practice matches it with ZCuSn5Pb5Zn5 in GB/T 1176, and Europe with EN 1982 CuSn5Pb5Zn5 (CC491K). Because US limits on lead and impurities differ from the Chinese and European ranges, a GB certificate does not automatically satisfy an ASTM B584 call-out.
| UNS | C83600 |
|---|---|
| Common name | 85-5-5-5 / 85 metal |
| ASTM | B584 (sand cast) / B505 (continuous cast) |
| SAE | J461 / J462 |
| China | ZCuSn5Pb5Zn5 (GB/T 1176) |
| Europe | CuSn5Pb5Zn5 / CC491K (EN 1982) |
Equivalent grades are close in composition and duty, not identical. Order and certify to the standard named on the drawing.
How to Specify C83600 on a Drawing
- State ASTM B584 and the casting process; if bar stock is wanted, state ASTM B505 instead.
- Add a pressure-tightness test where the part seals, and say what test pressure and medium apply.
- Require a chemical certificate that reports lead, because lead content drives both machinability and any potable-water restriction.
- Give machining allowance and datum faces; red brass castings move slightly during machining if the pattern is not well supported.
- If the part contacts drinking water, check the applicable lead rules first. C83600 is a leaded alloy and is no longer accepted for many potable-water fittings, where lead-free grades such as C89833 or C89835 are used instead.
Selecting C83600
Use C83600 when a casting must hold pressure, machine cleanly and resist water corrosion at moderate cost. For bearings, C93200 is the better choice. For cheap non-pressure fittings, C84400 with more zinc is common. Where lead is restricted - drinking water, food equipment, some export markets - the lead-free C89833/C89835 family is the modern substitute, at some cost in castability and machinability.
Casting and Machining Notes
C83600 is a forgiving casting alloy: it is fluid, feeds well with properly placed risers, and can be brazed or soldered. Welding is not recommended. Machining is rated at about 84% of free-cutting brass. The foundry points that matter are gas porosity and shrinkage in heavy sections, so gating and risering should be designed for directional solidification, and pressure castings should be tested rather than assumed sound.
Frequently asked questions about C83600
Why is C83600 called 85-5-5-5?
The name records the nominal composition: about 85% copper with 5% each of tin, lead and zinc. The UNS number C83600 is the formal designation; "85 metal", "ounce metal" and "red brass" are trade names for the same alloy.
Is C83600 allowed for drinking-water fittings?
Not in many markets. C83600 contains 4-6% lead, and potable-water rules such as NSF/ANSI 61 in the US and the EU drinking-water directive restrict lead leaching. Lead-free replacements C89833 and C89835 are specified instead. Always check the rule that applies to the destination market before quoting a leaded red brass for water service.
Can C83600 be welded?
Welding is not recommended: the lead phase volatilises and the weld zone is unsound. Brazing and soldering work well, and castings are normally joined mechanically or by brazing rather than by fusion welding.
C83600 or C84400 - which should I specify?
C84400 is a semi-red brass with more zinc and less tin and lead, so it is cheaper but weaker and less corrosion-resistant. C83600 is the better choice for pressure-containing and water-facing parts; C84400 suits low-cost, non-pressure fittings and decorative work.
Data compiled from published ASTM B505/B505M, B584 and B148 limits and from mill specification sheets; for selection reference only. Ordering is subject to the standard and the mill certificate. Data source: Shenyang Yuheng Metal Manufacturing Co., Ltd. — yuhengmetal.com.
Related grades
C93200 · C93700 · ZCuSn5Pb5Zn5 (GB/T 1176) | All grades in the library