Chemical Composition (%)
| Cu | 86.0-89.0 |
|---|---|
| Sn | 7.5-9.0 |
| Zn | 3.0-5.0 |
| Pb | 0.30 max |
| Ni | 1.0 max |
| Fe | 0.20 max |
| P | 0.05 max |
| Sb | 0.20 max |
| S | 0.05 max |
| Al / Si | 0.005 max each |
Limits as published for the ASTM designation; single values are maximums unless shown as a range. Cu is stated as the balance.
Mechanical & Physical Properties
| Tensile strength | 276-310 MPa (40-45 ksi) |
|---|---|
| Yield strength | 124-152 MPa (18-22 ksi) |
| Elongation | 18-30% |
| Hardness | 65-75 HB (typical) |
| Density | 8.80 g/cm³ |
| Machinability | 30 (free-cutting brass = 100) |
| Electrical conductivity | 12% IACS |
Minimum values are standard limits; hardness and machinability are typical values unless marked as minimum.

Typical Applications
Grade Overview
C90300 is the lead-free 88-8-0-4 tin bronze: about 88% copper, 8% tin and 4% zinc, with lead held to 0.30% maximum as an impurity rather than an alloying addition. It combines good strength with excellent corrosion resistance and pressure tightness, which is why it appears in pump bodies, valve bodies and steam fittings as readily as in bearings and gears. Published limits give 276-310 MPa tensile strength, 124-152 MPa yield strength, 18-30% elongation and 65-75 HB, with a machinability rating of about 30 against free-cutting brass. For buyers who must remove lead from a supply chain, C90300 is the usual first stop in the tin-bronze family.
The alloy is a single-phase alpha solid solution under normal casting conditions. Tin provides solid-solution strengthening; zinc improves fluidity and castability and lowers cost; nickel and iron, held to maxima, refine the structure. Because there are no deliberate lead particles, C90300 does not have the built-in lubricity or embeddability of a leaded bronze such as C93200. What it offers instead is better corrosion resistance, no lead-leaching route, and pressure tightness that suits castings which must hold water, steam or oil.

Microstructure and Behaviour
Under the microscope the structure is cored alpha with tin-rich and copper-rich regions. Slow cooling and heavy sections promote tin segregation and, at high tin levels, grain-boundary delta phase, both of which reduce ductility. Foundry practice therefore aims at uniform section thickness, controlled pouring temperature and adequate feeding. There is no hardening heat treatment; properties come from composition and sound casting, and stress relief is used only where machining distortion matters.
Standards and Equivalents
C90300 is ordered to ASTM B584 for sand castings, ASTM B505/B505M for continuous-cast rod and bar and ASTM B271 for centrifugal castings; SAE J461 and J462 list the same UNS number. The three product forms share the designation but differ in test-bar practice, section size and acceptance rules, so the purchase order should name the form as well as the UNS number. The closest GB/T 1176 designation is ZCuSn8Zn4; the two overlap in tin and zinc but are not identical, and a drawing written to one should not be swapped for the other without a composition check.
Selecting C90300
C90300 sits between the leaded bearing bronzes and the higher-tin wear grades. Against C93200 it gives up machinability (30 versus roughly 70) and embeddability, but gains corrosion resistance and removes lead from the part. Against C90500 it carries slightly less tin, so it is a little softer and more ductile. Against C90700 it is clearly softer (65-75 HB versus about 102 HB) and is not the grade for heavily loaded worm wheels. Choose C90300 for lead-free pump and valve castings, general-purpose bearings at moderate load, gears, piston rings and parts that must pass a pressure test.
How to Specify C90300 on a Drawing
- UNS number — C90300, not just "tin bronze".
- Product form and ASTM standard — B584 sand cast, B505 continuous cast or B271 centrifugal; each has different test requirements.
- Temper — as-cast (F) is normal; no solution or precipitation treatment applies.
- Test bars — specify separately cast test bars per the standard, and state whether tensile results are required per lot or per heat.
- Pressure tightness — for valve and pump bodies, state the hydrostatic test pressure and the acceptance criterion.
- Machining allowance — give finished dimensions, datum faces and any bearing bore tolerance such as H7 or H8.
Casting and Machining Notes
The wide freezing range means risers must feed the last solidifying section; put the riser where the section is heaviest and avoid isolated thin-to-thick transitions. Tin segregation responds to pouring temperature and cooling rate more than to stirring. C90300 welds only fairly and should not be repaired by welding on pressure-retaining surfaces. Machining at a rating of 30 needs sharp, positive-rake tooling and steady feeds; without lead to break the chip, stringy swarf and built-up edge are the usual problems.
Pressure tightness and valve service
Valve bodies, pump casings and steam fittings are the classic C90300 applications because the alloy combines a fine, sound casting structure with corrosion resistance in water and steam. For pressure-retaining parts, agree the hydrostatic test before casting: the test pressure, the hold time and whether leaking castings may be impregnated or must be scrapped. Impregnation is common for non-critical housings but is usually not accepted for valve bodies in safety-related service.
Frequently asked questions about C90300
Is C90300 lead-free?
Yes for practical purposes: lead is limited to 0.30% maximum as an impurity, with no deliberate addition. That is low enough for most lead-restriction programmes, but the acceptance limit depends on the end-use regulation, so ask for the certificate of analysis and check the actual figure rather than relying on the grade name.
C90300 or C90500 - which should I specify?
C90500 carries 9-11% tin against 7.5-9% in C90300, so it is slightly stronger and harder (70-80 HB versus 65-75 HB) with similar ductility. Both are lead-free. Choose C90300 for general pressure-tight castings and moderate bearings, C90500 where a little more hardness and wear resistance are wanted in the same family.
Can C90300 replace C93200 in a bearing?
Only after checking the duty. C93200 contains lead, machines at about 70 and embeds dirt well; C90300 is lead-free, machines at about 30 and has less embeddability. In clean, well-lubricated, moderate-load service the swap works; in dirty or starved lubrication the leaded grade usually lasts longer.
Which ASTM standard applies to my part?
Sand castings: ASTM B584. Continuous-cast bar and rod: ASTM B505/B505M. Centrifugal castings: ASTM B271. Name the form and the standard on the drawing; the UNS number alone does not define test bars, section limits or acceptance rules.
Can C90300 be used for steam fittings?
Steam fittings and valve bodies are traditional applications for this grade. For elevated-temperature design, ask the foundry for derating data at the intended temperature instead of assuming room-temperature properties apply.
Why is C90300 harder to machine than leaded bronze?
There is no lead phase to lubricate the cut and break the chip. Use sharp carbide tooling, positive rake, adequate coolant and steady feeds; avoid dwelling so the work does not work-harden. Expect lower metal-removal rates than with C93200 and plan machining cost accordingly.
Data compiled from published ASTM B584, B505/B505M and B271 limits and from mill specification sheets (Diversified Bronze, Concast, St. Paul Foundry); for selection reference only. Ordering is subject to the standard and the mill certificate. Data source: Shenyang Yuheng Metal Manufacturing Co., Ltd. — yuhengmetal.com.