Chemical Composition (%)
| Cu | 83.0 min |
|---|---|
| Al | 10.0-11.5 |
| Fe | 3.0-5.0 |
| Ni | 1.50 max |
| Mn | 0.50 max |
Limits as published for the ASTM designation; single values are maxima.
Mechanical & Physical Properties
| Tensile strength | >= 586 MPa (85 ksi) |
|---|---|
| Yield strength (0.5% ext.) | >= 221 MPa (32 ksi) |
| Elongation (2 in.) | >= 12% |
| Hardness | about 170 HB (typical) |
| Density | 7.45 g/cm3 |
| Melting range | 1027-1038 C |
| Electrical conductivity | 13% IACS |
| Machinability | about 60% of free-cutting brass |
Mechanical values are standard minima; hardness is typical.
Typical Applications
Bushings and bearings under high load, worm wheels, gears, valve bodies and seats, pump bodies and impellers, wear rings, marine propellers and hardware, and pressure-containing parts that must resist seawater. It is also chosen where a casting may need repair by welding.
Grade Overview
C95400 is the standard cast aluminum bronze of the US market, often called 9C. About 10-11.5% aluminum with 3-5% iron in a copper base gives it strength and hardness well above the tin bronzes, with good resistance to seawater, dilute acids and many process fluids. Iron refines the grain and forms hard particles that improve wear resistance, and the alloy can be heat treated to raise strength further.
It is used where a casting must be both a structural part and a wear surface: pump bodies and impellers, valve bodies and seats, worm wheels, gears, bearing retainers, wear rings and marine hardware. It is also one of the few cast copper alloys that can be welded, which matters for repairs and for building up worn surfaces.
Standards and Equivalents
ASTM B505 covers continuous-cast bar, ASTM B148 covers sand-cast aluminum bronze, and ASTM B271 covers centrifugal castings. QQ-C-390 G5 and MIL-B-16033 Class 3 are older call-outs still seen on drawings. GB/T 1176 lists ZCuAl10Fe3 as the nearest Chinese grade, and EN 1982 has CuAl10Fe3 (CC331G). Composition ranges and mechanical minima differ between these standards, so certify to the one named on the order.
| UNS | C95400 |
|---|---|
| Common name | 9C aluminum bronze |
| ASTM | B505 (continuous) / B148 (sand cast) / B271 |
| Federal / military | QQ-C-390 G5; MIL-B-16033 Class 3 |
| China | ZCuAl10Fe3 (GB/T 1176) |
| Europe | CuAl10Fe3 / CC331G (EN 1982) |
Equivalent grades are close in composition and duty, not identical. Order and certify to the standard named on the drawing.
How to Specify C95400 on a Drawing
- State the condition - as-cast or heat-treated (quench and temper) - because the mechanical values differ and the certificate must match the drawing.
- For pressure parts, add the pressure test and the casting-soundness requirements.
- If weld repair is permitted, say so and set the procedure and inspection; if it is not, say that too.
- Avoid specifying C95400 where the part runs against a hardened steel shaft at high speed with poor lubrication; it is less forgiving than the leaded bronzes.
Selecting C95400
C95400 is the choice when strength, wear resistance and seawater corrosion resistance are needed in one casting. For higher strength and better corrosion resistance in seawater, nickel aluminum bronze C95500 or C95800 is better. Where conformability and embeddability dominate, a leaded tin bronze such as C93200 or C93700 is more suitable. Where the part is a high-strength gear or valve stem and corrosion is not severe, C86300 manganese bronze is stronger still.
Casting and Machining Notes
C95400 needs controlled cooling: thick sections cooled slowly can precipitate brittle phases, and the alloy is sensitive to aluminum at the top of the range, so castings should be inspected for brittle structure before machining. It machines at about 60% of free-cutting brass, with sharp tooling and light cuts. It can be welded with a suitable procedure, but heat input, preheat and interpass temperature must be controlled; brazing is poor. When mating with steel, allow for the difference in thermal expansion and conductivity.
Frequently asked questions about C95400
Is C95400 weldable?
Yes, with a controlled procedure. Heat input, preheat and interpass temperature must be managed, and the weld area inspected, because aluminum bronze can crack or form brittle phases if cooled badly. Brazing, by contrast, is poor. Many foundries prefer weld repair to be agreed in writing before it is done.
C95400 or C95500 - which is stronger?
C95500 is a nickel aluminum bronze with roughly 4-5.5% nickel; it is stronger, harder and more corrosion-resistant in seawater, and it is the choice for propellers and heavy marine duty. C95400 is cheaper and easier to cast, and is adequate for most pump, valve and gear parts.
Can C95400 be heat treated?
Yes. Quench-and-temper treatment raises tensile and yield strength, and the drawing must state the condition because as-cast and heat-treated properties differ. Specify the condition and the test requirements together.
Does C95400 work in seawater?
It resists seawater well and is widely used in marine pumps, valves and hardware. For high-velocity seawater or critical parts, a nickel aluminum bronze is preferred. Isolate it from steel and other more noble metals where galvanic corrosion is possible.
Data compiled from published ASTM B505/B505M, B584 and B148 limits and from mill specification sheets; for selection reference only. Ordering is subject to the standard and the mill certificate. Data source: Shenyang Yuheng Metal Manufacturing Co., Ltd. — yuhengmetal.com.
Related grades
C86300 · ZCuAl10Fe3 (GB/T 1176) · ZCuAl10Fe3Mn2 (GB/T 1176) | All grades in the library